+高级检索
Monel-400合金高温力学性能及断裂行为分析
DOI:
作者:
作者单位:

内蒙古科技大学,包钢西北创业有限公司 包钢设计研究院,内蒙古科技大学,内蒙古科技大学,内蒙古科技大学

作者简介:

通讯作者:

中图分类号:

TG142.7

基金项目:

国家科技重大专项子课题项目(2009ZX04014-064-05);内蒙古科技大学材料与冶金学院青年人才孵化器平台项目


Analysis of High Temperature Mechanical Properties and Fracture Behaviors on Monel-400 Alloy
Author:
Affiliation:

Inner Mongolia University of Science and Technology,Baogang Design & Research Institute, Baogang Northwest Venture Industrial Development Co., Ltd,Material and Metallurgy School, Inner Mongolia University of Science and Technology,Material and Metallurgy School, Inner Mongolia University of Science and Technology,Material and Metallurgy School, Inner Mongolia University of Science and Technology

Fund Project:

  • 摘要
  • |
  • 图/表
  • |
  • 访问统计
  • |
  • 参考文献
  • |
  • 相似文献
  • |
  • 引证文献
  • |
  • 资源附件
  • |
  • 文章评论
    摘要:

    利用Gleeble-1500D热模拟机对不同温度下的Monel-400合金及熔敷金属进行拉伸试验。试验结果表明,母材和熔敷金属在高温下的强度不断下降,母材的塑性随温度的升高而增大,熔敷金属的塑性急剧下降。在高温下,细小弥散的第二相粒子对熔敷金属起到了明显的强化作用,而熔敷金属的塑性发生了严重劣化。母材从低温到高温(700~1100℃)的断裂形式是韧性断裂,熔敷金属断裂形式由韧性断裂逐步变为脆性断裂。在实际热加工和应用过程中,避免熔敷金属发生大变形,防止产生加工热裂纹,避免母材在700℃以上使用。

    Abstract:

    In order to investigate high temperature mechanical properties and fracture behaviors of Mone1-400 alloy and cladding metal tensile tests were conducted at different temperatures on a Gleeble-1500D thermal simulation machine. The results show that strength of base metal and cladding metal are declining from 700℃ to 1100℃. The plasticity of base metal increases with increasing temperature, while plasticity of the cladding metal declines. At 700℃, the dispersed second phase particles has played a significant role in strengthening the yield strength and tensile strength on the cladding metal, while plasticity of which is seriously deteriorated. At the range of 700 - 1100℃, the fracture pattern of base metal is ductile fracture, while fracture pattern of cladding metal from ductile fracture gradually become brittle fracture. In the actual thermal processing and application, it is crucial to avoid cladding metal large deformation to prevent thermal cracking, and the base metal should not be used above 700℃.

    参考文献
    相似文献
    引证文献
引用本文

陈重毅,王文君,麻永林,邢淑清,陆恒昌. Monel-400合金高温力学性能及断裂行为分析[J].稀有金属材料与工程,2016,45(7):1782~1787.[chenzhongyi, wangwenjun, mayonglin, xignshuqign, luhengchang. Analysis of High Temperature Mechanical Properties and Fracture Behaviors on Monel-400 Alloy[J]. Rare Metal Materials and Engineering,2016,45(7):1782~1787.]
DOI:[doi]

复制
文章指标
  • 点击次数:
  • 下载次数:
  • HTML阅读次数:
  • 引用次数:
历史
  • 收稿日期:2014-06-19
  • 最后修改日期:2014-07-17
  • 录用日期:2014-08-12
  • 在线发布日期: 2016-10-09
  • 出版日期: