+高级检索
粉末触变成形制备SiCp/2024p复合材料半固态组织的研究
DOI:
作者:
作者单位:

兰州理工大学 有色金属先进加工与再利用省部共建国家重点实验室,兰州理工大学 有色金属先进加工与再利用省部共建国家重点实验室,兰州理工大学 有色金属先进加工与再利用省部共建国家重点实验室,兰州理工大学 有色金属先进加工与再利用省部共建国家重点实验室

作者简介:

通讯作者:

中图分类号:

TB333

基金项目:

国家自然科学基金资助项目(G2010CB635106);兰州理工大学红柳杰出人才(J201103)


Research on Semi-Solid Microstructural Evolution of SiCP/2024pComposite Prepared by Powder Thixoforming
Author:
Affiliation:

State Key Laboratory of Advanced Processing and Recycling of Nonferrous Metals,Lanzhou University of Technology,State Key Laboratory of Advanced Processing and Recycling of Nonferrous Metals,Lanzhou University of Technology,State Key Laboratory of Advanced Processing and Recycling of Nonferrous Metals,Lanzhou University of Technology,State Key Laboratory of Advanced Processing and Recycling of Nonferrous Metals,Lanzhou University of Technology

Fund Project:

National Natural Science Foundation of China (51362017); Joint Fund of Jinchuan Company and Kunming University of Science and Technology (201101)

  • 摘要
  • |
  • 图/表
  • |
  • 访问统计
  • |
  • 参考文献
  • |
  • 相似文献
  • |
  • 引证文献
  • |
  • 资源附件
  • |
  • 文章评论
    摘要:

    提出粉末触变成形这一新技术。研究了SiCp/2024p压块在部分重熔中的组织演变,也讨论了加热温度和SiC含量(0%~20%)对半固态组织的影响。结果表明:5%SiCp/2024p压块在635℃加热0~60 min的组织演变分为三个阶段:初期2024p中晶粒的快速粗化、初生相周围液膜的形成,最后经球化形成触变成形所需细小、圆整的半固态浆料,对应的相变为θ→α,θ + α→L和α→L及α→L。适当升高温度,益于获得理想的半固态组织。SiCp减缓了组织演变速率。初生相的粗化速率很小,一个粉末演变成一个α-Al颗粒。

    Abstract:

    A new technology, powder thixoforming, has been proposed in this paper. Microstructural evolution during partial remelting of the SiCp/2024 aluminum composite prepared by cold pressing of alloy powders has been investigated. The effects of heating temperature and SiCp volume fractions (0%~20%) on semisolid microstructure have also been discussed. The results indicate that the microstructural evolution of the 5%SiCp/2024 composite can be divided into three stages, the initial rapid coarsening of the fine grains within 2024 powders, the formation of continuous liquid layer on the primary particle surface and finally formed the slurry needed by thixoforming with the small and spheroidal solid particles through the spheroidization during heating at 635℃ (0~60 min), which are attributed to the phase transformations of θ→α, θ + α→L and α→L, and α→L, respectively. Proper rising the partial remelting temperature is beneficial for obtaining ideal semisolid microstructure available for thixoforming. The microstructural evolution rate of the composites is slower than that of the matrix alloy. The coarsening rate of the primary particles is quite slow, one powder evolves into one primary particle with a continuous liquid layer surface.

    参考文献
    相似文献
    引证文献
引用本文

李普博,陈体军,陈玉狮,张素卿.粉末触变成形制备SiCp/2024p复合材料半固态组织的研究[J].稀有金属材料与工程,2017,46(6):1551~1558.[Li Pubo, Chen Tijun, Chen Yushi, Zhang Suqing. Research on Semi-Solid Microstructural Evolution of SiCP/2024pComposite Prepared by Powder Thixoforming[J]. Rare Metal Materials and Engineering,2017,46(6):1551~1558.]