+高级检索
7075-T6铝合金激光-MIG复合焊焊接接头疲劳寿命原位研究
DOI:
作者:
作者单位:

北京科技大学 新金属材料国家重点实验室,北京科技大学 新金属材料国家重点实验室,北京科技大学 新金属材料国家重点实验室,西南交通大学 牵引动力国家重点实验室

作者简介:

通讯作者:

中图分类号:

基金项目:

国家自然科学基金项目(面上项目,重点项目,重大项目)


Investigation of fatigue lifetime of Laser-MIG hybrid welded joint of 7075-T6 aluminum alloy by in-situ observation
Author:
Affiliation:

State Key Laboratory for Advanced Metals and Materials,University of Science and Technology Beijing,State Key Laboratory for Advanced Metals and Materials,University of Science and Technology Beijing,State Key Laboratory for Advanced Metals and Materials,University of Science and Technology Beijing,State Key Laboratory of Traction Power,Southwest Jiaotong University

Fund Project:

  • 摘要
  • |
  • 图/表
  • |
  • 访问统计
  • |
  • 参考文献
  • |
  • 相似文献
  • |
  • 引证文献
  • |
  • 资源附件
  • |
  • 文章评论
    摘要:

    本文对7075-T6铝合金激光复合焊焊接接头的疲劳寿命进行了探究。结果表明:疲劳裂纹萌生寿命与疲劳寿命之间存在着一定的比例关系。对于母材试样,该比值为64.5%;而对于焊接接头试样,该比值为20.2%。疲劳断口表面观察发现,母材试样的疲劳断口上存在大量韧窝,而焊接接头试样疲劳断口上存在许多气孔。这些气孔被认为是引起焊接接头疲劳裂纹萌生寿命急剧下降的主要原因。

    Abstract:

    The fatigue lifetime of the laser-MIG hybrid welded joint of 7075-T6 aluminum alloy was studied in this paper. The results showed that there existed a strong relationship between the fatigue crack initiation lifetime and fatigue failure lifetime. For the base metal specimens the ratio of fatigue crack initiation lifetime and fatigue failure lifetime was about 64.5%, while for the welded joint specimens it was about 20.2%. The observation of fatigue fracture surface showed that there existed a large number of dimples in the base metal specimens, while there appeared lots of gas porosities in the welded joint specimens instead. These gas porosities were regarded to be the reason of lower fatigue crack initiation lifetime.

    参考文献
    相似文献
    引证文献
引用本文

张寅,宋西平,常丽艳,吴圣川.7075-T6铝合金激光-MIG复合焊焊接接头疲劳寿命原位研究[J].稀有金属材料与工程,2017,46(9):2411~2416.[Zhang Yin, Song Xiping, Chang Liyan, Wu Shengchuan. Investigation of fatigue lifetime of Laser-MIG hybrid welded joint of 7075-T6 aluminum alloy by in-situ observation[J]. Rare Metal Materials and Engineering,2017,46(9):2411~2416.]
DOI:[doi]

复制
文章指标
  • 点击次数:
  • 下载次数:
  • HTML阅读次数:
  • 引用次数:
历史
  • 收稿日期:2015-09-25
  • 最后修改日期:2015-10-21
  • 录用日期:2015-11-18
  • 在线发布日期: 2017-11-29
  • 出版日期: