+高级检索
Si对异步轧制Cu/Al-Si复合板界面组织及性能影响
DOI:
作者:
作者单位:

东北大学材料电磁过程研究教育部重点实验室,东北大学材料电磁过程研究教育部重点实验室,东北大学材料电磁过程研究教育部重点实验室,东北大学材料电磁过程研究教育部重点实验室

作者简介:

通讯作者:

中图分类号:

基金项目:

国家自然科学基金资助(51174058)


Study of Silicon on Microstructure, Mechanical Properties of Asymmetric Roll Bonded Cu/Al-Si Alloy Clads
Author:
Affiliation:

Key Laboratory of National Education Ministry for Electromagnetic Processing of Materials,Northeastern University,Key Laboratory of National Education Ministry for Electromagnetic Processing of Materials,Northeastern University,Key Laboratory of National Education Ministry for Electromagnetic Processing of Materials,Northeastern University,Key Laboratory of National Education Ministry for Electromagnetic Processing of Materials,Northeastern University

Fund Project:

  • 摘要
  • |
  • 图/表
  • |
  • 访问统计
  • |
  • 参考文献
  • |
  • 相似文献
  • |
  • 引证文献
  • |
  • 资源附件
  • |
  • 文章评论
    摘要:

    在异步速比为1.7的异步轧制工艺下冷轧制备Cu/Al-Si复合板,不同Si含量的Cu/Al-Si复合板在400℃退火30min后界面获得均匀厚度的金属间化合物。利用OM、SEM、EPMA、XRD、拉伸机等设备分析发现:复合板金属间化合物的厚度在Si含量为8.66%时最大;随着Si含量的增加,复合板的抗拉强度增大,延伸率、剥离强度减小,在Si含量为4.84%时综合性能最好,抗拉强度和延伸率分别为188.63MPa、39.1%;Cu侧的拉伸断口形貌主要呈山脊状,Al-Si合金侧中心区域出现韧窝,韧窝数量随Si含量增加而增加。

    Abstract:

    Cu/Al-Si alloy clads were cold roll bonded with a mismatch speed ratio of 1.7 at ambient temperature, and uniform intermetallic compounds(IMCs) formed when these Cu/Al-Si alloy laminates with different silicon content were annealed at 400 ℃ for 30 minutes. With the utilizition of OM, SEM, EPMA, XRD, tensile machine and so on, it showed that the width of IMCs reached the maximum at 8.66%(wt.%) silicon content. With increase of silicon in Al-Si alloy, the tensile strength of laminated composites increased while elongation and peeling strength of composites went down, and their comprehensive properties reached the best at 4.84% with tensile strength and elongation of 188.63 MPa、39.1%, respectively. Meanwhile, fracture morphology of Cu/Al-Si alloy laminates in Cu side was ridge-like, and structure of Al-Si alloy in center region was mainly dimples, the more silicon content in Al-Si alloy, the more dimples appealed.

    参考文献
    相似文献
    引证文献
引用本文

刘国平,王平,赵莹莹,常东旭. Si对异步轧制Cu/Al-Si复合板界面组织及性能影响[J].稀有金属材料与工程,2018,47(1):223~228.[Liu Guoping, Wang Ping, Zhao Yingying, Chang Dongxu. Study of Silicon on Microstructure, Mechanical Properties of Asymmetric Roll Bonded Cu/Al-Si Alloy Clads[J]. Rare Metal Materials and Engineering,2018,47(1):223~228.]