High Temperature Steam Oxidation Behavior of Cr-coated Zr Fabricated by Filtered Cathodic Vacuum Arc Ion Deposition
Author:
Affiliation:

1.Key Laboratory of Beam Technology of Ministry of Education,College of Nuclear Science and Technology,Beijing Normal University;2.Beijing Radiation Center

Fund Project:

Nuclear Materials Innovation Foundation (ICNM-2020-YZ-04), Beijing Natural Science Foundation (2172029) and National Natural Science Foundation of China (51671032)

  • 摘要
  • |
  • 图/表
  • |
  • 访问统计
  • |
  • 参考文献
  • |
  • 相似文献
  • |
  • 引证文献
  • |
  • 资源附件
  • |
  • 文章评论
    摘要:

    采用磁过滤阴极真空弧离子镀(FCVAD)技术在纯锆表面制备了厚度约为4 μm的Cr金属层,对比研究了它们在不同温度水蒸汽环境中的氧化行为,并利用XRD、XPS、SEM及EDS分析了Cr涂层及氧化膜的物相组成、微观结构及成分分布。结果表明,在900℃、1000℃和1100℃水蒸汽环境中,镀Cr涂层大幅度降低了锆的氧化速率,其单位面积氧化增重仅为同一温度下锆基体的1/4、1/6和4/9。氧化初期,Cr涂层表面生成一层均匀致密的Cr2O3膜,当Cr层被消耗完后,Cr2O3/Zr界面上部分Cr2O3被Zr还原成金属Cr,锆基体氧化生成ZrO2。镀Cr涂层样品的氧化激活能达293.17 kJ/mol。

    Abstract:

    A Cr coating of about 4 μm thick was successfully prepared on pure zirconium by filtered cathodic vacuum arc ion deposition technology (FCVAD), and the high-temperature oxidation properties of bare and Cr-coated Zr were measured using a thermogravimetric analyzer (TGA) in steam environment at different temperatures. Their phase composition, microstructure and composition distributions before and after the steam oxidation tests were characterized by X-ray diffraction analyzer (XRD), X-ray photoelectron spectroscopy (XPS), scanning electron microscope (SEM) and energy dispersive X-ray spectroscopy (EDS). It was found that the mass gain per unit area of Cr-coated Zr was only 1/4, 1/6 and 4/9 of that of bare Zr after 3600 s exposure in 900, 1000 and 1100℃ steam environment, respectively. In the initial stage of steam oxidation, a compact and uniform Cr2O3layer was formed on the surface of Cr layer, significantly reducing oxygen or steam diffusion inwards. After Cr coating was completely oxidized into Cr2O3, Zr substrate was gradually oxidized, but the Cr2O3 at Cr2O3/Zr interface was reduced to form Cr. In addition, the oxidation activation energy of the Cr-coated Zr was up to 293.17 kJ/mol.

    参考文献
    相似文献
    引证文献
引用本文

王兴平,魏克俭,廖斌,关浩浩,陈琳,杜建成,徐驰,薛文斌.锆表面磁过滤阴极真空弧离子镀Cr涂层高温蒸汽氧化行为研究[J].稀有金属材料与工程,2021,50(5):1665~1672.[Wang Xingping, Wei Kejian, Liao Bin, Guan Haohao, Chen Lin, Du Jiancheng, Xu Chi, Xue Wenbin. High Temperature Steam Oxidation Behavior of Cr-coated Zr Fabricated by Filtered Cathodic Vacuum Arc Ion Deposition[J]. Rare Metal Materials and Engineering,2021,50(5):1665~1672.]
DOI:10.12442/j. issn.1002-185X.20200372

复制
文章指标
  • 点击次数:
  • 下载次数:
  • HTML阅读次数:
  • 引用次数:
历史
  • 收稿日期:2020-05-30
  • 最后修改日期:2020-06-25
  • 录用日期:2020-07-01
  • 在线发布日期: 2021-06-09
  • 出版日期: 2021-05-25