+高级检索
添加YbZrAl7Si0.3Mg合金组织及力学性能的影响
作者:
作者单位:

1.昆明理工大学 材料科学与工程学院,云南 昆明 650093;2.昆明冶金研究院有限公司,云南 昆明 650031;3.西南石油大学工程学院,四川 南充 637001

作者简介:

通讯作者:

中图分类号:

基金项目:

Major Science and Technology Project in Yunnan Province-New Material Special Project (202102AB080004,2018ZE005,2019ZE001); Yunnan Province Transformation Research Institute Technology Development Research Project-Innovation Guidance and Technology Enterprise Cultivation Plan (202102AB080004)


Effect of Yb and Zr Addition on Microstructure and Mechanical Properties of Al7Si0.3Mg Alloy
Author:
Affiliation:

1.Faculty of Materials Science and Engineering, Kunming University of Science and Technology, Yunnan 650093, China;2.Kunming Metallurgy Research Institute Company Limited, Yunnan 650031, China;3.School of Engineering, Southwest Petroleum University, Nanchong 637001, China

Fund Project:

Major Science and Technology Project in Yunnan Province-New Material Special Project (202102AB080004, 2018ZE005, 2019ZE001); Yunnan Province Transformation Research Institute Technology Development Research Project-Innovation Guidance and Technology Enterprise Cultivation Plan (202102AB080004)

  • 摘要
  • |
  • 图/表
  • |
  • 访问统计
  • |
  • 参考文献
  • |
  • 相似文献
  • |
  • 引证文献
  • |
  • 资源附件
  • |
  • 文章评论
    摘要:

    研究了添加Yb和Zr元素对Al7Si0.3Mg合金组织及力学性能的影响,以及细化变质机理。结果表明,Yb、Zr元素的添加明显细化了α-Al基体,使其从粗大的树枝状晶转变为细小的花瓣状晶,晶粒尺寸明显减小,并且使共晶硅由粗大的针状变质为短棒状,这是由于Yb、Zr吸附在孪晶凹槽处(TPRE)改变共晶硅生长方式,最终改变共晶硅形貌;经热处理(T6)后,大量析出的Al3(Yb, Zr)粒子起到了沉淀强化进而细化晶粒的作用。当Yb质量分数为0.3%、Zr质量分数为0.25%时,合金(T6)的抗拉强度和延伸率为296.3 MPa和9.2%,较未细化变质的合金分别提高了17%和1.1倍。

    Abstract:

    The effects of adding Yb and Zr elements on the microstructure and mechanical properties of Al7Si0.3Mg alloy and the mechanism of refinement and modification were investigated. The results show that the addition of Yb and Zr elements can significantly refine the α-Al matrix, transforming it from coarse dendritic crystals to fine petal-like crystals with a significant reduction in grain size, and the eutectic silicon metamorphoses from coarse needle-like to short rod-like. The modification mechanism of eutectic silicon is that the adsorption of Yb and Zr at the twin grooves (TPRE) changes the eutectic silicon growth mode and finally changes the eutectic silicon morphology. After heat treatment (T6), a large number of Al3(Yb, Zr) particles are precipitated to strengthen and refine the grain, and the addition of Yb and Zr can significantly improve the mechanical properties of the alloy. The tensile strength and elongation of the alloy (T6) are 296.3 MPa and 9.2% when the Yb content is 0.3wt% and the Zr content is 0.25wt%, which are 17% and 1.1 times higher than those of the unrefined and unmodified alloy, respectively.

    参考文献
    相似文献
    引证文献
引用本文

吉全鑫,杜景红,张艺杰,李玉章,冯炜光,孙彦华,严继康,甘国友.添加YbZrAl7Si0.3Mg合金组织及力学性能的影响[J].稀有金属材料与工程,2022,51(10):3580~3587.[Ji Quanxin, Du Jinghong, Zhang Yijie, Li Yuzhang, Feng Weiguang, Sun Yanhua, Yan Jikang, Gan Guoyou. Effect of Yb and Zr Addition on Microstructure and Mechanical Properties of Al7Si0.3Mg Alloy[J]. Rare Metal Materials and Engineering,2022,51(10):3580~3587.]
DOI:10.12442/j. issn.1002-185X.20210908

复制
文章指标
  • 点击次数:
  • 下载次数:
  • HTML阅读次数:
  • 引用次数:
历史
  • 收稿日期:2021-10-19
  • 最后修改日期:2021-12-27
  • 录用日期:2022-01-29
  • 在线发布日期: 2022-10-31
  • 出版日期: 2022-10-28