+高级检索
亚微米活化Mo-15Cu合金晶间反应机制
作者:
作者单位:

1.哈尔滨理工大学 材料科学与工程学院,哈尔滨 150040;2.哈尔滨工程大学 智能科学与工程学院,哈尔滨 150006

作者简介:

通讯作者:

中图分类号:

基金项目:

中央支持地方高校改革发展资金项目,项目名称:脉冲电流作用下镁基材料烧结/锻造关键技术研究,项目编号:323210001;哈尔滨人才项目,项目名称:钼铜合金电触头熔渗工艺研究,项目编号:2015RAQXJ036


Intergranular Reaction Mechanism of Submicron-Activated Mo-15Cu Alloy
Author:
Affiliation:

1.School of Materials Science and Chemical Engineering, Harbin University of Science and Technology, Harbin 150040, China;2.College of Intelligent Systems Science and Engineering, Harbin Engineering University, Harbin 150006, China

Fund Project:

Project supported by the Reform and Development of Local Colleges and Universities of the Central Government of China (323210001); Project supported by the Harbin Talents of China (2015RAQXJ036)

  • 摘要
  • |
  • 图/表
  • |
  • 访问统计
  • |
  • 参考文献
  • |
  • 相似文献
  • |
  • 引证文献
  • |
  • 资源附件
  • |
  • 文章评论
    摘要:

    为了研究具有亚微米组分的钼铜粉末烧结时的晶间反应机制,采用亚微米活化层法制备了一种具备晶间反应层的钼铜复合材料。采用X射线衍射仪(XRD)、扫描电镜(SEM)、能谱仪(EDS)、透射电镜(TEM)、高分辨透射电镜(HRTEM),对Mo-15Cu合金组织形貌、连接和结构特征进行了表征。研究了亚微米活化层对钼铜复合材料晶间反应的影响。结果表明,添加8%(质量分数)亚微米粉,可形成厚度约0.5 μm纳米活化层。Mo亚微米颗粒通过流动、扩散,改变晶间反应机制,形成了真正意义上的晶间反应层,厚度约为5 nm,实现了冶金结合。

    Abstract:

    In order to investigate the intergranular reaction mechanism during sintering of molybdenum-copper powders with submicron components, a Mo-15Cu composite with an intergranular reaction layer was prepared by a submicron-activated layer method. The histomorphology, connectivity and structural characteristics of Mo-15Cu alloy were characterized by X-ray diffracto-meter (XRD), scanning electron microscope (SEM), energy dispersive spectrometer (EDS), transmission electron microscope (TEM), and high-resolution transmission electron microscope (HRTEM). The effect of submicron-activated layers on the intergranular reaction of Mo-15Cu composites was investigated. The results show that the submicron-activated layer with a thickness of 0.5 μm is formed by adding 8wt% submicron powder. The submicron-sized Mo particles change the intergranular reaction mechanism through flow and diffusion, forming an intergranular reaction layer with a thickness of about 5 nm and achieving metallurgical bonding.

    参考文献
    相似文献
    引证文献
引用本文

王敬泽,尹佳庆,崔建文,常晶,于彦东,孙云龙.亚微米活化Mo-15Cu合金晶间反应机制[J].稀有金属材料与工程,2023,52(2):448~453.[Wang Jingze, Yin Jiaqing, Cui Jianwen, Chang Jing, Yu Yandong, Sun Yunlong. Intergranular Reaction Mechanism of Submicron-Activated Mo-15Cu Alloy[J]. Rare Metal Materials and Engineering,2023,52(2):448~453.]
DOI:10.12442/j. issn.1002-185X.20220244

复制
文章指标
  • 点击次数:
  • 下载次数:
  • HTML阅读次数:
  • 引用次数:
历史
  • 收稿日期:2022-03-23
  • 最后修改日期:2023-02-08
  • 录用日期:2022-06-17
  • 在线发布日期: 2023-03-03
  • 出版日期: 2023-02-28