+高级检索
时效处理对Ti-6Al-3Nb-2Zr-Mo合金组织演变和力学性能的影响
作者:
作者单位:

1.中国科学院金属研究所 核材料与安全评估重点实验室;2.中国科学技术大学 材料科学与工程学院;3.中国科学院金属研究所 沈阳材料科学国家实验室

作者简介:

通讯作者:

中图分类号:

基金项目:

National Key Research and Development Program [Grant No. 2018YFA0702900], National Natural Science Foundation of China [Grant Nos. 52173305, 52101061, 52233017, 52203384], Strategic Priority Research Program of the Chinese Academy of Sciences [Grant No. XDC04000000], China Postdoctoral Science Foundation [Grant Nos. 2020M681004, 2021M703276], IMR Innovation Foundation [Grant No. 2022-PY12], LingChuang Research Project of China National Nuclear Corporation, and Youth Innovation Promotion Association, CAS.


Effects of Aging Treatment on Microstructure Evolution and Mechanical Properties of Ti-6Al-3Nb-2Zr-Mo Alloy
Author:
Affiliation:

1.Key Laboratory of Nuclear Materials and Safety Assessment, Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China;2.School of Materials Science and Engineering, University of Science and Technology of China, Shenyang 110016, China;3.Shenyang National Laboratory for Materials Science, Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China

Fund Project:

National Key Research and Development Program (2018YFA0702900); National Natural Science Foundation of China (52173305, 52101061, 52233017, 52203384); Strategic Priority Research Program of the Chinese Academy of Sciences (XDC04000000); China Postdoctoral Science Foundation (2020M681004, 2021M703276); IMR Innovation Foundation (2022-PY12); LingChuang Research Project of China National Nuclear Corporation; Youth Innovation Promotion Association, CAS

  • 摘要
  • |
  • 图/表
  • |
  • 访问统计
  • |
  • 参考文献
  • |
  • 相似文献
  • |
  • 引证文献
  • |
  • 资源附件
  • |
  • 文章评论
    摘要:

    为了解不同时效参数对Ti-6Al-3Nb-2Zr-Mo (Ti6321)合金组织和力学性能影响的根本原因,通过光学显微镜(OM)、扫描电镜(SEM)、透射电镜(TEM)和力学性能测试,研究了不同时效条件(500~650 ℃,3~24 h)下的显微组织和力学性能。结果表明,次生相ααs)比初生相ααp)对时效参数更为敏感。此外,αs相的厚度与时效温度和时效时间呈正相关。随着时效温度和时效时间的增加,Ti和Al元素在βt相中的偏析明显,αs相由细针状转变为长棒状。当合金在600 ℃时效12 h时,合金表现出较好的综合力学性能。抗拉伸强度、屈服强度和伸长率分别为907 MPa、796 MPa和16%,冲击功为55 J。

    Abstract:

    In order to understand the influence of the different aging parameters on the microstructure and mechanical properties of Ti-6Al-3Nb-2Zr-Mo (Ti6321) alloy, the microstructures and mechanical properties under different aging parameters (temperatures ranging from 500 °C to 650 °C, 3–24 h) were investigated by optical microscopy (OM), scanning electron microscopy (SEM), transmission electron microscopy (TEM), and mechanical properties tests. The results reveal that the secondary α phase (αs) is more sensitive to the aging parameters than the primary α phase (αp). Moreover, the thickness of αs phase is positively correlated with aging temperature or aging time. As the aging temperature and aging time increase, the segregation of Ti and Al elements in the β transformation phase (βt) becomes obvious, and the αs phase changes from fine needle-like to long rod-like. When the alloy is aged at 600 °C for 12 h, the alloy shows good comprehensive mechanical performance. The tensile strength, yield strength, and elongation are 907 MPa, 796 MPa, and 16%, respectively, and the impact energy is 55 J.

    参考文献
    相似文献
    引证文献
引用本文

江海洋,江福清,王冰,徐斌,孙明月.时效处理对Ti-6Al-3Nb-2Zr-Mo合金组织演变和力学性能的影响[J].稀有金属材料与工程,2023,52(6):2002~2009.[Jiang Haiyang, Jiang Fuqing, Wang Bing, Xu Bin, Sun Mingyue. Effects of Aging Treatment on Microstructure Evolution and Mechanical Properties of Ti-6Al-3Nb-2Zr-Mo Alloy[J]. Rare Metal Materials and Engineering,2023,52(6):2002~2009.]
DOI:10.12442/j. issn.1002-185X.20220943

复制
文章指标
  • 点击次数:
  • 下载次数:
  • HTML阅读次数:
  • 引用次数:
历史
  • 收稿日期:2022-12-04
  • 最后修改日期:2023-02-07
  • 录用日期:2023-02-14
  • 在线发布日期: 2023-07-03
  • 出版日期: 2023-06-30