K439B铸造高温合金双态型γ相长期时效粗化行为研究
作者:
作者单位:

1.北京科技大学 新金属材料国家重点实验室, 北京 100083;2.中国航发北京航空材料研究院 先进高温结构材料重点实验室, 北京 100095

作者简介:

通讯作者:

中图分类号:

TG132.33

基金项目:

国家科技重大专项(J2019-VI-0004-0117);先进高温结构材料重点实验室基金项目(6142903220101);国家重点研发计划(2022YFB3706804)


Coarsening Behavior of Bimodal γ′ Phase in K439B Cast Superalloy During Long-Term Aging
Author:
Affiliation:

1.State Key Laboratory of Advanced Metals and Materials, University of Science and Technology Beijing, Beijing 100083, China;2.Science and Technology on Advanced High Temperature Structural Materials Laboratory, Beijing Institute of Aeronautical Materials, Beijing 100095, China

Fund Project:

National Science and Technology Major Project of China (No. J2019-VI-0004-0117),Science and Technology on Advanced High Temperature Structural Materials Laboratory Fund (No. 6142903220101),National Key Research and Development Program of China (No. 2022YFB3706804)

  • 摘要
  • |
  • 图/表
  • |
  • 访问统计
  • |
  • 参考文献
  • |
  • 相似文献
  • |
  • 引证文献
  • |
  • 资源附件
  • |
  • 文章评论
    摘要:

    以承温能力达800 ℃的K439B合金为研究对象,研究该合金标准热处理态组织中γ′相的形态,以及800 ℃下时效6000、7000、8000和10000 h过程中的γ′相演变规律和粗化行为。结果表明,合金标准热处理后枝晶干γ′相细小均匀,而枝晶间γ′相呈现出大小两种形态。合金在长期时效后枝晶间区域仍然保留双态型γ′相。合金长期时效后γ′相由标准热处理态的球状逐渐向立方状转变,立方状γ′相获得了互相平行的边界,未出现筏排化现象。合金在长期时效过程中,γ′相尺寸增大,但体积分数变化不明显。γ′相尺寸随时效时长的变化同时符合Lifshitz-Slyozov-Wagner(LSW)和相界面扩散控制理论(TIDC)两种模型,其内在原因认为是由于元素在基体与界面的扩散速率相当。

    Abstract:

    This article took K439B alloy with a temperature bearing capacity of 800 ℃ as the research object to study the γ′ phase morphology in the standard heat-treated condition, and the γ′ phase evolution and coarsening behavior during aging at 800 ℃ for 6000, 7000, 8000, and 10 000 h. The results indicate that the γ′ phase at the dendrites in the alloy is fine and uniform, while the γ′ phase between the dendrites presents two types. After long-term aging, the bimodal γ′ phase is still retained in the interdendritic region, and the γ′ phase transforms from spherical to cubic shape without any rafting phenomenon. During the long-term aging process, the γ′ phase size of the K439B increases, but the change in volume fraction is not significant. The variation of γ′ phase size with aging time conforms to both Lifshitz-Slyozov-Wagner (LSW) and theory of interface diffusion control (TIDC) models. The internal reason is believed to be the equivalent diffusion rate of elements between the matrix and interface.

    参考文献
    相似文献
    引证文献
引用本文

屈星海,高磊,吴一栋,惠希东,肖程波,陈晶阳.K439B铸造高温合金双态型γ相长期时效粗化行为研究[J].稀有金属材料与工程,2025,54(2):490~496.[Qu Xinghai, Gao Lei, Wu Yidong, Hui Xidong, Xiao Chengbo, Chen Jingyang. Coarsening Behavior of Bimodal γ′ Phase in K439B Cast Superalloy During Long-Term Aging[J]. Rare Metal Materials and Engineering,2025,54(2):490~496.]
DOI:10.12442/j. issn.1002-185X.20230721