Abstract:The effect of indium ion concentration, current density and continuous electrolysis time on the purity and size of the powder by electrolysis process was studied. The results show that:Continuous electrolysis time is longer, the larger sizes of the powder were obtained when the electric parameters are: NaCl concentration is 80g/L, polar distance is 5 cm, thiourea concentration is 0.3 g/L, gelatin concentration is 0.5 g/l, pH = 2.5, Polyvinyl ketone(PVP) is 0.2 g/L. When the current density is 130 A/m2, the particle size of the powder is the smallest, and the purity is the highest. The effect of In3+ concentration on the particle size is the least, but the influence on the purity is the most. Under the conditions of process parameters above and In3+ concentration of 30 g/L, the current density of 130 A/cm2, electrolytic for 1h, the particle size of less than 100 μm indium powder were obtained, which the particle size of less than 30 μm accounted for 75%.